PROJECT RESULT
The raw ore was ground with a fineness of -200 mesh accounted for 70.1%. The gold grade reached 335.4g/t-348.7g/t and the gold recovery rate of heavy sand 1 was 53.51%-56.31% through gravity separation by shake table. Heavy sand 1 contained granular gold with a gold grade of 30.2g/t-43.51g/t, and heavy sand 2 can be obtained with a gold recovery rate of 9.0%-10.41%. The flotation gold ore with a gold grade of 24.26g/t-29.38g/t and recovery rate of 25.85%-29.05% could be obtained from the tailings of gravity separation by flotation. The recovery rate of gold in the beneficiation test of gravity separation and flotation process reached 91.56%-92.57%.