Xinhai xinhai-cu-pb-zn-ore-dressing-process Ore Dressing Process
It is reported that more than 90% of non-ferrous metal ores (copper, lead, zinc, etc.) adopt flotation process, especially for those with fine grain and complex symbiosis. Flotation process can achieve ideal separation effect, and separately recover low-grade ore then enrich multiple high-grade concentrates. Different ore properties means different flotation process. According to the dissemination characteristics of metal minerals, Xinhai has determined four kinds of flotation processes:
Key Point: Lead-Zinc Separation, Copper-Zinc Separation, Copper-Lead Separation
In general, the most difficulty of the polymetallic sulfide ores separation is the separation among several kinds of ores, especially those low-graded ores with complex embedded features. Therefore, it’s a significant step for separating lead-zinc, copper-zinc, copper-lead to choose right flotation reagents. Xinhai strictly implements the reagent system, controls the dosage of reagent, reduces multiple circulation and loss, then strengthens the flotation effect.
01
Lead-Zinc Ore Separation
Differential flotation process, floats lead and depresses zinc.
Collectors: Low-level xanthate, advanced xanthate, aerofloat. Separation in alkaline medium.
Inhibitor: CN-、NaCN、kCN、ZnSO4、Na2OS3、Na2S2O3
02
Copper-Zinc Separation
Differential flotation process, floats copper and depresses zinc. If the separating difficulty is over 2, the depression on zinc should be strengthened.
Collectors: Low-level xanthate, advanced xanthate, aerofloat. Separation in alkaline medium.
Inhibitor: CN-、NaCN、kCN、ZnSO4、Na2OS3、Na2S2O3
03
Copper-Lead Separation
Dereagent first, then differential flotation process. Floats copper and depresses lead, or floats lead and depresses copper.
Floats copper and depresses lead: Widely used in secondary copper ore, Cu2+ ions are dissolved too much and bot easy to be inhibited.
Inhibitor: Knox reagent(K2CrO4+KCrO2) combined with Na2S, or oxysulfide.
Floats lead and depresses copper: Widely used in primary copper ore.
Collectors: xanthate, aerofloat. Keep PH value among 9-605, then adjust with CaO.
Inhibitor: cyanide and other inhibitors, or hot dereagent to inhibit lead (40~70℃, and PH value≤7).